MENINGKATKAN CBR DAN MEMPERKECIL SWELLING TANAH SUB GRADE DENGAN METODE STABILISASI TANAH DAN KAPUR Warsiti Jurusan Teknik Sipil Politeknik Negeri Semarang Jln. Prop. Soedarto, SH Tembalang Semarang
[email protected] Abstract The condition of Sendang Mulyo road is not good and always be damaged even though the coating of road surface has been carried out. This is due to the fact that road internodes of Sendang Mulyo locates on the clay, so that it may causes instability of base soil causing structure destruction of coarsening layer on it. In order to solve the problem, the base soil should be repaired/destabilized. In this research, the writer conducted soil stabilization by adding lime from Purwodadi. The aim of the research is to find out the lime percentage, so that CBR and max dry density will be obtained, to find out the effect of lime adding with Swelling (kembang susut) and California Bearing Ratio (CBR). The testing was performed at the laboratory with lime percentage of 0%, 5%, 8%, 10%, 12%. The testing data includes: physical characteristics (specific gravity, Plasticity Index, decrease limit, grain pass from the filter no.200)., mechanical characteristics (optimum water degree, maximum dry density, CBR, Swelling). Dry density increases from 1,485% to 1,64%, From data analysis, it was obtained the result that in lime percentage of 10% produces CBR scale experiencing maximum increase from 2,45% to 7,6%, swelling decreases from 5,127% to 1,331%. The effect of lime adding upon swelling may be written as follows y = -0,0109X2 – 0,2469X + 5,2528, (y = swelling, x = lime percentage), the effect of lime adding with CBR is y = -0,0766X2 + 3,6352X + 2,3048 (y = CBR, x = lime percentage). Keywords : CBR, Lime, Swelling, Stabilization
PENDAHULUAN Salah satu kekuatan atau kekokohan suatu konstruksi ditentukan oleh kwalitas bahan dasar yang dipergunakan. Seperti pada suatu konstruksi jalan, kualitas tanah asli sebagai bahan dasar (subgrade) juga sangat menentukan kekuatan jalan. Jika tanah asli mempunyai daya dukung (kepadatan kering, CBR) rendah, maka konstruksi jalan akan cepat mengalami kerusakan. Kondisi jalan di daerah Sendang Mulyo juga mengalami hal yang sama, yaitu cepat mengalami kerusakan meskipun sering dilakukan perbaikan pada permukaan (lap surfase). Untuk mengatasi permasalahan tersebut salah satu cara atau metode yang dipergunakan adalah memperbaiki kualitas tanah asli (stabilisasi). Hasil penelitian yang dilakukan oleh Andrews dan Oflaherty (Satrio, 1998), 38
menunjukkan bahwa kapur lebih efektif sebagai bahan stabilisator tanah dari pada semen, dan dapat dipakai untuk berbagai jenis tanah. Suryolelono (1999) menyatakan penambahan abu sekam padi dan kapur juga meningkatkan sudut gesek dalam tanah. Stabilisasi dengan kapur dan posolan cocok untuk tanah kohesif (Soedarmo dan Purnomo, 1997 dalam Wiqoyah, 2002). Penelitian yang pernah dilakukan adalah stabilisasi tanah Sendang Mulyo dengan kapur Purwodadi, tetapi yang ditinjau baru kerapatan kering (γd) saja. Dari hasil penelitian yang pernah dilakukan adalah tanah Sendang Mulyo termasuk jenis tanah lempung dan mempunyai kepadatan kering (γd) maksimum 1,483964 t/m3, hasil penelitian stabilisasi tanah dengan kapur adalah kepadatan kering (γd) maksimum 1,633448 (t/m3), pada persentase kapur optimum = 10,80769 (%) dan dengan kadar air = 19 (%) (Warsiti, 1998).
Dari permasalahan tersebut mendorong peneliti untuk melakukan penelitian lebih lanjut tentang pengaruh stabilisasi tanah dengan kapur terhadap besarnya California Bearing Ratio ( CBR ) dan swelling (muai dan susut). Tanah lempung mempunyai sifat-sifat yang tidak menguntungkan, seperti Bearing Ratio (CBR) rendah, kembang susut (swelling) tinggi sehingga apabila dipergunakan untuk tanah dasar (subgrade) jalan akan menghasilkan suatu konstruksi yang tidak optimal hasilnya (cepat rusak). Untuk itu, jika akan dipergunakan suatu konstruksi sebaikan nilai Bearing Ratio dinaikkan agar mampu menahan beban di atasnya, kembang susut (swelling) diturunkan agar volume tanah stabil bila kena hujan tidak mengembang sebaliknya bila musim kemarau tidak meyusut terlalu tinggi sehingga retak-retak pada jalan bisa dikurangi atau dihilangkan. Kriteria yang dipakai untuk menilai memuaskan atau tidaknya stabilisasi, didasarkan faktor kekuatan dengan menggunakan parameter kepadatan kering maksimum (γd) dan CBR, swelling. CBR merupakan ukuran daya dukung tanah yang dipadatkan dengan daya pemadatan tertentu dan kadar air tertentu dibandingkan dengan beban standard pada batu pecah. Dengan demikian, besaran CBR adalah persentase atau perbandingan daya dukung tanah yang diteliti dan daya dukung batu pecah standar pada nilai penetrasi yang sama (0,1 inch dan 0,2 inch). CBR laboratorium diukur dalam dua kondisi, yaitu kondisi tidak terendam disebut CBR Unsoaked dan kondisi terendam atau disebut CBR soaked. Pada umumnya CBR soaked lebih rendah dari CBR Unsoaked. Namun demikian kondisi soaked adalah kondisi yang serinng dialami di lapangan, sehingga di dalam perhitungan konstruksi bangunan, harga CBR soaked yang dipergunakan sebagai dasar perhitungan karena dalam kenyataannya air selalu mempengaruhi konstruksi bangunan. Potensi pengembangan tanah dengan berbagai nilai indeks plastisitas (IP) dapat dilihat dalam Tabel 1. Ada dua alasan lempung lebih diperhatikan. Pertama, cukup banyak masalah
tanah dalam praktik perekayasaan dan salah satunya masalah lempung. Yang kedua, kapur hanya efektif sebagai bahan stabilisasi pada tanah yang mengandung lempung cukup banyak. Tabel 1. Tentang Potensi Pengembangan Berbagai Nilai Indeks Plastisitas Indeks Plastisitas Potensi Pengembangan (PI) 0 – 15 Rendah 10 – 20 Sedang 20 – 35 Tinggi > 35 Sangat tinggi Sumber : Chen, 1975 (dalam Lashari, 2000)
Tujuan penelitian adalah menjelaskan pengaruh penambahan kapur ke dalam tanah terhadap peningkatan CBR (daya dukung tanah), swelling, dan mengetahui persentase kapur optimum sehingga diperoleh CBR maksimum dan swelling minimum. METODE PENELITIAN Untuk menyelesaikan penelitian ini diperlukan beberapa tahapan, yaitu a) tahapan pendahuluan,dalam hal ini meliputi mempersiapkan material yang akan dipergunakan seperti pengambilan sampel tanah Sendang Mulyo dan kapur dari Purwodadi, b) dilanjutkan studi literatur, seperti mempelajari penelitian sejenis yang pernah dilakukan, teori-teori yang menunjang tentang stabilisasi tanah, metode-metode memperbaiki tanah, prosedur pengujian, dan teknik analisis data, c) pengujian laboratorium dimulai dari mempersiapkan bahan uji menimbang persentase kapur, mencapur tanah dengan masing-masing persentase kapur, kemudian dimasukkan ke dalam plastis dan diperam selama tiga hari, pengujian CBR dan Swelling untuk masing-masing persentase kapur sebanyak lima pengujian(Tabel 2). % kapur 0% 5% 8% 10% 12%
Tabel 2. Matrik Data CBR X01 X02 X03 X04 X11 X22 X23 X24 X31 X32 X33 X34 X41 X42 X43 X44
X05 X25 X35 X45
X51
X55
X52
MENINGKATKAN CBR DAN MEMPERKECIL SWELLING TANAH……..(Warsiti )
X53
X54
39
Begitu juga untuk data swelling, jumlahnya sama, yaitu 25 buah. Prosedur berikutnya adalah analisis data. Analisis ini meliputi kompilasi data, membuat regresi hubungan antara persentase kapur dan besarnya CBR, regresi hubungan antara persentase kapur dan besarnya swelling, menghitung besarnya persentase kapur optimum agar diperoleh CBR maksimum dan swelling minimum dari regresi yang terbentuk. Untuk lebih jelas metode penelitian dapat dilihat dalam Gambar 1. Diagram alur penelitian. Program Kerja
Persiapan: Pengambilan Sampel Tanah di Sendang Mulyo, kapur dari Purwodadi
Studi Literatur
Pengujian Tanah Asli dan Campuran tanah + Kapur , Konsentrasi Kapur : 5%, 8%, 10%, 12%, dengan lama pemeraman 3 hari
Dalam menganalisis data dilakukan tahapan sebagai berikut, yaitu a) melakukan kompilasi data yaitu mengelompokkan data ke dalam masing-masing kelompok sesuai dengan persentase kapur yang dipergunakan, b) menentukan nilai rata-rata hasil uji CBR dan swelling dari maisng-masing persentase kapur, c) menentukan regresi hubungan antara prosentase kapur dan CBR dan menentukan persamaan regresinya, d) menentukan regresi antara persentase kapur dan swelling, e) menguji korelasi antara prosentase kapur dengan CBR dan Swelling, dan menentukan prosentase optimum agar diperoleh CBR maksimum dan swelling minimum berdasarkan regresi yang diperoleh. HASIL Hasil Pengujian Tanah Asli Pengujian laboratorium mengenai karakteristik fisik tanah asli meliputi berat jenis, batas-batas Atterberg (batas cair, batas plastis, plasticity index, bata susut) dan analisis distribusi butiran dengan hasil seperti pada Tabel 3. Pengujian sifat mekanis, yaitu kepadatan, CBR, dan nilai kembang susut (swelling) dilakukan dengan metode pemadatan Standard Proctor. Hasil pengujian dapat dilihat pada Tabel 4. Hasil percobaan laboratorium . Tabel. 3. Karakteristik Fisik Tanah Asli
Uji CBR Laboratorium, Swelling
AnalisIs Data: - Kompilasi data - Regresi antara % kapur dengan CBR dan Swelling - Menentukan %kapur maksimum agar CBR maksimum & Swelling minimum
Kesimpulan
Gambar 1. Diagram Alur Penelitian
40
Pemeriksaan Berat jenis (t/m3) Batas cair (LL) Batas plastis (PL) Batas susut (SL) Plasticity index (PI) Lempung (lolos saring no.200)
Hasil 2,49 57,95% 24,48% 18,82% 33,47% 60,75%
Dari hasil pengujian fisik di atas dapat dikatakan bahwa jika tanah dengan LL = 4060 % , PI = 25-41 % menurut Chen (1975) tanah tersebut tergolong tingkat pengembangan tinggi sehingga berdasarkan pendapat tersebut maka tanah asli dapat dikatakan tanah lempung yang mempunyai tingkat pengembangan tinggi
Wahana TEKNIK SIPIL Vol. 14 No. 1 April 2009: 38-45
Tabel 4. Karakteristik mekanis tanah asli Hasil Pengujian Campuran Tanah Asli dengan Kapur
Standard Proctor 24 % 1,485 t/m3 11.8 2.45 97.97 5,127
Pemeriksaan Kadar air optimum (OMC) Kepadatan kering max CBR unsoacked (%) CBR soaked (%) Derajat kejenuhan (%) Swellinng Potensial (%)
Pengujian dilakukan terhadap beberapa campuran tanah lempung dan bahan stabilisasi kapur dengan berbagai komposisi campuran ( 0 %, 5%, 8%, 10%, 12%). Pengujian tersebut meliputi pengujian sifat-sifat mekanis berupa pengujian pemadatan, CBR, swelling.
Untuk pengujian analiisa distribusi butir dilakukan dengan percobaan analisis saringan dan percobaan analisis hydrometer. Hasil percobaan analisis saringan seperti terlihat pada Tabel 5 dan Gambar 2, yang menunjukkan bahwa 60,75% butiran lolos saringan No.200. Tabel. 5. Hasil pengujian analisa saringan Ukuran Saringan Inc mm h No
Berat tertingga l (gram)
Jumlah
Jumlah
Lolos
tinggal
tinggal
Saringan
(gram)
(%)
(%)
0
0
0
100
0
0
0
100
4
4.76
8
2.38
10
2.00
1.71
1.71
0.86
99.15
20
0.59
5.73
7.44
3.72
96.28
40
0.42
10.53
17.97
8.99
80
Hasil penelitian CBR dan swelling adalah sebagai berikut (Tabel 6- 9). Tabel 6. Hasil Uji CBR Unsoaked dengan Berbagai Persentase Kapur % Kapur
CBR unsoaked (%)
Rerata
0%
11.9
11.82
11.91
11.52
11.84
11.8
5%
13.27
14.02
12.93
13.26
13.03
13.3
8%
18.75
18.56
17.88
18.35
18.46
18.4
10%
22.63
21.97
21.82
22.35
21.72
22.1
12%
22.24
22.11
21.8
21.58
22.27
22
Tabel 7. Hasil uji CBR soaked dengan berbagai prosentase kapur
91.02
% Kapur 0%
5.035
5.201
5.057
5.206
5.136
5.127
82.93
5%
4.289
4.186
4.206
4.326
4.263
4.254
Swelling potensial (%)
Rerata
0.177
16.18
34.15
17.08
100
0.149
17.72
51.87
25.94
74.07
8%
2.238
2.305
2.243
2.245
2.204
2.247
200
0.074
26.64
78.51
39.26
60.75
10%
1.351
1.308
1.325
1.354
1.317
1.331
12%
1.028
1.134
0.982
1.006
0.975
1.025
120
Tabel 8. Uji Swelling dengan berbagai prosentase kapur
Berat Lolos Saringan (%)
100
Jenis penelitian Kd air opt(%)
80
60
40
20
0 0,01
0,10
1,00
10,00
0%
Prosentase kapur 5% 8% 10 %
12 %
Kpdt kering mak
24.0
21.6
19.8
17.10
19.2
CBR unsoaked (%)
1,580
1,62
1,65
1,64
CBR soaked (%)
1,49 11,8
13.3
18.4
22.1
22
Kd air opt (%)
2,45
3.6
5.1
7.6
7.58
Swell potensial (%)
5,13
4,25
2,25
1,331
1,025
100,00
Diam e ter Butir (m m )
Gambar 2. Grafik distribusi ukuran butiran
Regresi Variabel Bebas dan Takbebas Dalam penelitian ini ditentukan variabel takbebas meliputi CBR, swelling, sedangkan variabel bebas adalah kadar kapur (% kapur).
MENINGKATKAN CBR DAN MEMPERKECIL SWELLING TANAH……..(Warsiti )
41
Grafik hubungan prosentase kapur dengan CBR 25 y = 0.0437x 2 + 0.4587x + 11.402 R2 = 0.9229
20 CBR (%)
CBR unsoaked
15
CBR soaked y = 0.0242x 2 + 0.187x + 2.3471 R2 = 0.9373
10 5 0 0
5 10 Prosentase kapur (%)
15
Gambar 3. Grafik hubungan prosentase kapur dengan CBR Regresi antara CBR dengan persentase kapur dalam campuran dapat dilihat dalam Gambar 3 diatas. Dari gambar di atas dapat dikatakan bahwa bentuk regresi yang dihasilkan sudah cukup sesuai/cocok karena R2 yang didapat mendekati 1(satu). Persamaan antara CBR dan persentase kapur dalam campuran adalah sebagai berikut. #. CBR dalam kondisi unsoaked y = 0,0437 X2 + 0.4587 X + 11,402 R2 = 0,9229, dimana : Y : CBR unsoaked (%) X : prosentase kapur (%) Dari hasil regresi yang diperoleh bahwa besarnya CBR maksimum meningkat terus dengan bertambahnya kadar kapur dalam campuran. #. CBR dalam kondisi soaked y = 0,0242 X2 + 0, 187 X + 2,3471 R2 = 0,9373, di mana : Y : CBR soaked (%) X : persentase kapur (%)
42
Dari hasil regresi yang diperoleh bahwa besarnya CBR akan mengalami kenaikan dengan meningkatnya kadar kapur dalam campuran. Hasil pengujian swelling menghasilkan penurunan swelling yang cukup tinggi. Swelling tanah asli sebesar 5,127 %, tetapi begitu tanah dicampur dengan kapur besar swelling mengalami penurunan seiring dengan penambahan persentase kapur. Penurunan yang terbesar terjadi pada persentase kapur sebesar 12 %, penurunan yang terjadi sebesar =(5,127-1,025)/5,127 * 100 % = 80 %. Jadi, dapat disimpulkan dengan penambahan akan memperbaiki tanah asli karena memperkecil besarnya swelling. Yang berarti merubah dari tanah yang mempunyai swelling tinggi menjadi tanah yang mempunyai swelling rendah. Adapun regresi hubungan antara besarnya swelling dengan prosentase kapur dalam campuran dapat dilihat dalam Gambar 4 berikut.
Wahana TEKNIK SIPIL Vol. 14 No. 1 April 2009: 38-45
Grafik % kapur dengan swelling 6 5,5
sw elling(%)
5 4,5 4 3,5 3 2,5 2
y = -0,0109x 2 - 0,2469x + 5,2528 R2 = 0,9536
1,5 1 0,5 0 0
2
4
6
8
10
12
14
% kapur (%)
Gambar 4. Grafik hubungan prosentase kapur dengan swelling Regresi hubungan antara swelling dan persentase kapur adalah sebagai berikut. y = -0,0109 X2 - 0,2469 X + 5,2528 R2 = 0,9536, di mana : Y : besarnya swelling (%) X : persentase kapur (%) Bentuk regresi yang dihasilkan sudah sesuai/baik hal ini dapat dilihat dari besarnya R2 mendekati 1 (satu). PEMBAHASAN Pengujian Tanah Asli Dari hasil pengujian sifat mekanis tanah asli yang meliputi kadar air optimum, kepadatan kering maksimum dan CBR maka dapat dikatakan tanah mempunyai daya dukung (CBR) rendah, yaitu 2,45 %. Syarat CBR tanah subgrade suatu konstruksi jalan adalah minimal 3 %. Dengan demikian, tanah tersebut tidak dapat dipergunakan untuk konstruksi sebagai lapisan subgrade karena CBR < 3%. Hasil pengujian swelling didapat tanah asli mempunyai swelling sebesar 5%, menurut Chen (1975) tanah yang mampunyai swelling>5% tergolong tanah dengan swelling potensial tinggi.
Pengujian Campuran Tanah Asli dengan Kapur Hasil pengujian CBR dengan metode standar terhadap tanah yang dicampur dengan kapur dari berbagai persentase dapat dikatakan CBR yang dihasilkan mengalami peningkatan yang cukup tinggi. Hasil pengujian CBR dalam kondisi unsoaked akan mengalami perbaikan dari 11.88% menjadi 22,1 % pada persentase kapur 10%. Begitu pula hasil CBR dalam kondisi soaked mengalami peningkatan yang cukup besar, yaitu dari 2,45 % menjadi 7,6 % pada persentase kapur 10 %. Dengan nilai CBR dalam kondisi soaked 7,6 % maka tanah campuran ini dapat dipergunakan sebagai lapisan subgrade- nya > 3 %. Dari bentuk dapat dikatakan bahwa bentuk regresi yang dihasilkan sudah cukup sesuai karena R2 yang didapat mendekati 1 dan dapat dikatakan besarnya CBR maksimum meningkat terus dengan bertambahnya kadar kapur dalam campuran. Hasil pengujian swelling menghasilkan penurunan swelling yang cukup tinggi. Swelling tanah asli sebesar 5,127 %, tetapi begitu tanah dicampur dengan kapur besar
MENINGKATKAN CBR DAN MEMPERKECIL SWELLING TANAH……..(Warsiti )
43
swelling mengalami penurunan seiring dengan penambahan persentase kapur. Penurunan yang terbesar terjadi pada persentase kapur sebesar 12 %, penurunan yang terjadi sebesar =(5,127-1,025)/5,127 * 100 % = 80 %. Jadi, dapat disimpulkan dengan penambahan akan memperbaiki tanah asli karena memperkecil besarnya swelling. Yang berarti mengubah dari tanah yang mempunyai swelling tinggi menjadi tanah yang mempunyai swelling rendah. Bentuk regresi yang dihasilkan sudah sesuai/baik hal ini dapat dilihat dari besarnya R2 mendekati 1 (satu). SIMPULAN Berdasarkan hasil pengujian, sifat fisik contoh tanah asli yang diambil pada ruas jalan Susukan–Kalikayen, mempunyai persentase sifat berikut, yaitu batas cair (LL) : 57,95 %, indeks plastisitas (PI) : 33,47 %, Batas Plastis (PL) : 24,48 %, batas susut : 18,52 %, dan lolos saringan No. 200 : 60,75 %. Data tersebut, menurut Chen (1975) digolongkan sebagai lempung dengan potensi pengembangan tinggi, dan menurut pusat penelitian dan pengembangan Teknologi Prasarana Jalan (2000) menunjukkan korelasi potensi pengembangan tinggi, sedangkan menurut Atterberg (1911) tingkat plastisitas tanah digolongkan sebagai lempung sangat plastis. Berdasarkan hasil pengujian mekanis dengan metode standar tanah asli mempunyai data berikut, yaitu kadar air optimum : 24 %, kepadatan maksimum : 1,485 %, CBR unsoacked : 11,8 %, CBR soacked : 2,45 %, dan swelling : 5,127 %. Dari data pengujian mekanis tersebut dapat dikatakan bahwa tanah mempunyai kepadatan, CBR rendah, sehingga tidak dapat dipergunakan untuk bahan subgrade jalan karena CBR-nya < 3.0 %. Untuk itu, apabila ingin dipergunakan untuk konstruksi sebagai subgrade tanah harus diberi perlakuan yaitu stabilisasi. Dengan demikian, dapat disimpulkan bahwa tanah asli merupakan tanah lempung dengan plastisitas tinggi, tingkat pengembangan tinggi serta potensi swelling tinggi., sehingga kurang baik bila dipergunakan secara langsung untuk konstruksi subgrade jalan. 44
Tanah asli dicampur dengan kapur dengan berbagai prosentase (5, 8, 10, 12 %), lama pemeraman 0 hari dan pegujian dilakukan dengan metode Standard Proctor. Berdasarkan pengujian sifat-sifat mekanik tanah campuran dengan metode tersebut dapat disimpulkan sebagai berikut: a. CBR keadaan unsoacked mengalami kenaikan dengan bertambahnya persentase kapur dalam campuran sampai pada persentase 10 %, dari 11,8 % menjadi 22,1 %, tetapi pada persentase kapur 12% CBR turun sedikit menjadi 22,0 %. Hubungan antara prosentase kapur dengan CBR keadaan unsoaked adalah y = 0,0437 X2 + 0.4587 X + 11,402. b. CBR keadaan soacked mengalami kenaikan dengan bertambahnya persentase kapur dalam campuran sampai pada persentase 10 %, dari 2,45 % menjadi 7,6 %, tetapi pada persentase kapur 12% CBR turun sedikit menjadi 7,58 %. Hubungan antara prosentase kapur dengan CBR keadaan soacked adalah y = 0,0242 X2 + 0, 187 X + 2,3471 c. Besarnya swelling mengalami penurunan dengan bertambahnya persentase kapur dengan kata lain semakin banyak prosentase kapur semakin kecil swelling yang terjadi. Hubungan antara persentase kapur dengan swelling adalah y = -0,0109 X2 - 0,2469 X + 5,2528 Berdasarkan hasil pengujian pengujian sifat fisik dan mekanis dari campuran tanpa pemeraman kepadatan kering (γd), CBR keadaan unsoaked dan soaked terbesar dicapai pada prosentase kapur 10%, maka dapat diambil kesimpulan bahwa yang paling baik untuk stabilisasi tanah lempung adalah dengan penambahan kapur 10 %. UCAPAN TERIMA KASIH Penulis mengucapkan terima kasih kepada Direktur Polines, UP2M Polines, Kalab Material Jurusan Sipil, serta rekan-rekan yang telah membantu dalam pelaksanaan penelitian ini.
Wahana TEKNIK SIPIL Vol. 14 No. 1 April 2009: 38-45
DAFTAR PUSTAKA Budi Satrio.1998. Kapur Argojati dalam Stabilisasi Tanah. Tesis Program Sistem dan Teknik Jalan Raya. ITB. Bandung. Chen, F.H, 1975. Founddation on Expansive Soil. New York: Elsevier Science Publishing Company. Lashari, 2000. Pengaruh Campuran Kapur dan Bubuk Bata Merah pada Sifat Mekanis Tanah Lempung Grobogan. Tesis UGM Yogyakarta. Suryolelono, K.B, 1999. “Potensi Variasi Campuran Abu sekam Padi dan Kapur untuk Meningkatkan Karakteristik Tanah Lempung” Jurnal Teknik, Volume VI, No.3, Desember.
Warsiti, 1998. Perbaikan Tanah Lempung dengan Kapur dari Daerah Sendang Mulyo Semarang: Laporan penelitian. Semarang. Politeknik Negeri semarang. Wiqoyah,Q, 2002. Campuran Kapur dan Tras Sebagai Bahan Stabilisasi Tanah Lempung Hitam untuk Lapisan Tanah Dasar Jalan. Naskah Seminar Hasil Penelitian Tesis S-2, Program Studi Teknik Sipil, Jurusan Ilmu-ilmu Teknik, Program Pascasarjana UGM. Yogyakarta.
MENINGKATKAN CBR DAN MEMPERKECIL SWELLING TANAH……..(Warsiti )
45